A trouble and measures of the whetstone

The abrasion of the whetstone is early
 
   A state: Oversight
     Cause
       ● Abrasive depth of the cut is big (per nothing drink)
       ● Bond is soft
       ● The dilution magnification of the grinding fluid is high
     Processing condition
       ● I lower the forwarding speed
       ● I raise whetstone number of revolutions
       ● I lower the depth of the cut
     Whetstone
       ● I raise a particle size
       ● I give an intensive degree
       ● I harden bond
     Grinding fluid
       ● I lower dilution magnification (I raise density)
 
Load gradually grows big, and processing is not continued
 
   A state: Close eyes
     Cause
       ● Abrasive depth of the cut is small
       ● Bond is hard
       ● The dilution magnification of the grinding fluid is low
     Processing condition
       ● I give forwarding speed
       ● I lower whetstone number of revolutions
       ● I give depth of the cut
     Whetstone
       ● I lower a particle size
       ● I lower the intensive degree
       ● I soften bond
     Grinding fluid
       ● I raise dilution magnification (I lower density)
   A state: Blocking
     Cause
       ● Grinding fluid does not arrive to a processing thing and the contact point of the whetstone
          ● Grinding fluid is polluted
       ● chippupoketo of the whetstone is small
     Processing condition
       ● I lower whetstone number of revolutions
     Whetstone
       ● I change a shape (I put a slit)
       ● I lower a particle size
       ● I lower the intensive degree
       ● I soften bond
 
     Grinding fluid
       ● I raise supply pressure
       ● Change
 
Tipping is easy to be given to the processing thing
 
     Cause
       ● Abrasive depth of the cut is big
     Processing condition 
       ● I lower the forwarding speed
       ● I raise whetstone number of revolutions
       ● I lower the depth of the cut
     Whetstone
       ● I raise a particle size
       ● I give an intensive degree
     Grinding fluid
       ● I lower dilution magnification (I raise density)
 
 
 